화학공학소재연구정보센터
Journal of Crystal Growth, Vol.490, 6-10, 2018
Growth of bulk ZnO crystals by self-selecting CVT method
Bulk ZnO crystals were grown by self-selecting CVT method using carbon as the transport agent. The crystal growth process took place on the top of the polycrystalline source material, and deep-red colored ZnO crystals of several millimeters were obtained. The as-grown crystals were characterized by X-ray diffraction (XRD), Energy Dispersive Spectrometer (EDS), Raman scattering (RS) spectroscopy, visible-near infrared (VIS-NIR) spectrophotometer and room temperature photoluminescence (PL) spectroscopy. XRD results indicate good crystallinity of the ZnO crystal. The EDS analysis shows that the crystal has a stoichiometry ratio Zn: O = 52: 48. The results suggest the existence of native defects of oxygen vacancies (OV) in the as-grown ZnO samples, which is caused by the stoichiometry shift to Zn-rich. (C) 2018 Published by Elsevier B.V.