Journal of the American Ceramic Society, Vol.93, No.7, 1916-1921, 2010
Electrophoretic Deposition of Ti3Si(Al)C-2 from Aqueous Suspension
Ti3Si(Al)C-2 films were electrophoretically deposited at 3 V on indium-tin-oxide (ITO) conductive glass from Ti3Si(Al)C-2 aqueous suspension with 1 vol% solid loading at pH 9 in the absence of any dispersant. The surface morphology, cross section microstructure, and preferred orientation of the films were investigated by scanning electron microscopy and X-ray diffraction. The as-deposited Ti3Si(Al)C-2 films exhibited (00l) preferred orientation and the thickness can be controlled by the deposition-drying-deposition method. These results demonstrate that electrophoretic deposition is a simple and feasible method to prepare MAX-phases green films at room temperature.