Indian Journal of Chemical Technology, Vol.17, No.5, 381-385, 2010
Electrolytic deposition of Zn-Mn-Mo alloys from a citrate bath
Zn-Mn-/vlo alloys were electrodeposited from a citrate bath and the influence of various parameters such as current density, 2.0-6.0 Adm(-2); temperature, 20-35 degrees C; pH, 2.0-2.15; duration of deposition 20-50 min and concentration of the constituent metals were studied. The electrolytic bath consists of zinc sulphate (20-35 gL(-1)), manganese sulphate (50-80 gL(-1)), ammonium molybdate (3-6 gL(-1)), citric acid (5 gL(-1)) and starch (1 gL(-1)). Semi bright, light gray adherent deposits were generally obtained containing 88.98-99.82% Zn, 0.06-8.70% Mn and 0.10-2.32% Mo. The variation of cathode polarization with current density or the pH under the conditions was studied. Morphological studies have also been done.